Defect · structure
Cavity wall tie corrosion
Steel ties in early cavity walls rust, expand, crack the bed joints, and stop tying the two leaves. In a high wind that can be more than a crack.
Mechanism
Cavity walls depend on ties. BRE found that steel ties made before 1981 could lose their protective coating well before the life expected of the wall, faster in black-ash mortar and in coastal exposure. Rust occupies more volume than steel, so the outer leaf cracks horizontally at the courses where the ties sit, often in a regular pattern, and can bow or lift. The inner leaf may look fine. Replacement is a surveyed installation of remedial stainless ties, not a bead of mastic in the crack.
Often confused with
- Subsidence cracks, which tend to be diagonal and to open doors out of square
- Thermal movement cracks at a long wall with no movement joint
- Lintol failure, which is a crack over one opening rather than a pattern up the wall
What would support it
- The wall is actually a cavity wall, built before the change to more durable ties
- Horizontal cracks in bed joints, repeating up the wall, perhaps with bowing
- Corroded ties seen with a borescope or by opening up, not assumed from the pavement
What would rule it out
- The wall is solid, or it is a timber frame with slips and no ties
- The ties are stainless and the cracks are hairline at a movement-joint position
- One diagonal crack after a dry summer, with no horizontal pattern
Common mistakes to avoid
- Do not buy tie replacement for a solid wall or a timber frame
- Do not fill the cracks and leave the leaves unconnected
- Do not assume a modern insulated cavity has 1960s wire ties
Frequently asked
Do repeating horizontal bed-joint cracks mean corroding wall ties?
They are the leading hypothesis on a pre-1981 cavity wall, especially with black-ash mortar or coastal exposure — rust expands and prises the outer-leaf bed joints at the tie courses in a regular vertical spacing (BRE Good Repair Guide 4 / Digests 329 and 401). Confirm the wall is a cavity, date the construction, and prove ties with a metal detector, borescope, or opening-up; do not diagnose from the pavement alone. Solid walls, timber-frame slips, lintol cracks over one opening, and movement-joint omissions are different mechanisms. Horizontal, repeating, sometimes with bowing of the outer leaf → investigate ties. One diagonal crack after a dry summer → clay/subsidence path, not ties.
How wide and patterned must cracks be before wall-tie corrosion is the leading hypothesis?
Pattern beats absolute width. Leading signs are multiple horizontal cracks aligned with tie courses up the elevation, often at roughly 450 mm or 900 mm vertical centres depending on the original tying schedule, sometimes with outer-leaf lift or bowing. Hairline cracks at a designed movement joint, or a single crack over a window head, are not enough. On post-1980s walls with stainless ties the same look is more often thermal movement or lintols — cut the score and instruct an invasive investigation before quoting full replacement (BRE Good Repair Guide 4; Digests 329 and 401). Map the crack grid on elevation drawings, measure widths for the record, but specify remedial stainless ties only after corroded ferrous ties are evidenced. Filling cracks and leaving the leaves untied is not a repair.
Remedies
- EstablishedReplace corroded cavity wall ties
When ties have corroded or were never adequate, the outer leaf is no longer reliably connected. The established repair is a survey of the ties and installation of remedial stainless ties, isolating the old ones where the specification requires it.
- EstablishedRecord cracks properly
Tell-tales, dated photographs with a scale, and a note of doors that stick. Digest 251 asks what repair the damage would need, not merely how wide one crack is. A single visit cannot show whether movement has stopped.